The below information is as far as we know, just for your reference only.
Type
of
Plastic
Resin
|
Pre-drying
(oC)
|
Melting
Temp.
(oC)
|
Injection
Pressure
(kg/cm2)
|
Screw
Speed
(rpm)
|
Mould
Temp.
(oC)
|
Shrinkage
Rate
(%)
|
Regrind
Ratio
(%)
|
Clamping
Force
(ton/in2)
|
AS
|
70-85;
1hr.
|
180-250
|
50-120
|
50-120
|
40-70
|
0.2-0.7
|
0
|
2
|
ABS
|
75-90;
1.5 hr.
|
180-250
|
60-120
|
70-100
|
40-75
|
0.4-0.7
|
15-25
|
2
|
GPPS
|
60-80;
1hr.
|
170-250
|
50-100
|
60-100
|
50-70
|
0.2-0.8
|
0
|
2
|
HIPS
|
60-90;
1hr.
|
175-220
|
60-110
|
60-100
|
55-75
|
0.2-0.8
|
15-25
|
2
|
PP
|
N/A
|
180-270
|
50-120
|
60-90
|
40-70
|
1.0-3.0
|
15-30
|
2
|
PE
|
N/A
|
180-250
|
50-100
|
60-100
|
35-55
|
1.5-3.5
|
15-40
|
2
|
PMMA
|
80-90;
a2hr.
|
220-240
|
80-140
|
60-80
|
55-75
|
0.2-1.0
|
0
|
4
|
PVC
|
N/A
|
180-210
|
70-120
|
60-90
|
40-60
|
Hard:
1-1.5;
Soft: 2-2.3
|
15-25
|
2
|
PC
|
90-110;
2hr.
|
260-320
|
70-120
|
40-60
|
70-95
|
0.5-0.7
|
10-25
|
4-6
|
PA
|
80-90;
4hr.
|
255-285
|
70-100
|
60-80
|
60-90
|
0.6-2.0
|
10-35
|
3-4
|
POM
|
N/A
|
175-210
|
50-100
|
50-80
|
60-80
|
2-3.0
|
10-50
|
4-5
|
PSF
|
120-140;
4-6hr.
|
300-360
|
80-130
|
80-130
|
85-140
|
0.5-0.7
|
10-30
|
6
|
PBT
|
80-120;
3-4hr.
|
240-260
|
80-130
|
60-80
|
50-70
|
1.7-2.3
|
10-30
|
3-4
|
CA
|
70-90;
1-4hr.
|
195-225
|
60-100
|
60-100
|
50-85
|
0.2-0.7
|
5-15
|
2-3
|
PPO
|
75-90;
1.5-3hr.
|
240-280
|
70-120
|
70-90
|
60-80
|
0.5-0.7
|
10-25
|
2-3
|
PET
|
130-150;
4-5hr.
|
250-275
|
50-80
|
50-70
|
90-120
|
1.5-2.5
|
10-30
|
4-6
|